Addition of hardeners
(A665, A666, A667)
Application: use a suitable knife or spreader. Apply one or more coats as necessary, allowing 5 –
10 minutes at 20°C between coats. Galvaplast 77 can be used directly on the bare metal.
Dry to sand:
from °C to 10°C
from 10 °C to 20 °C
from °C to 30°C
IR medium
IR short
Dry sanding paper grades:
Overcoating at 20° C:
Primer Deltron D821 – 2K HS Chip Resistant [low VOC Primer Surfacer]
D104 /For detailed information see technical datasheet "104 – Deltron D821"
For detailed information see chapter / section "Sanding and Cleaning"
Hardener and thinner selection: for detailed information see chapter / section "Hardeners and
Thinners"
Mixing Ratio
Untinted
D821
HS-Hardener
Thinner
Tinted
D821
DG
HS-Hardener
Thinner
Number of coats: 2-3
Flash-off between coats at 20°C: 10 – 15 minutes
Flash-off before stoving at 20°C: 10 – 15 minutes
Drying times:
Dustfree at 20°C
Touch dry at 20°C
Through dry at 20°C
Through dry at 60°C
Through dry (IR)
Total dry film build: 70 – 110 µm (tinted: 60 – 90 µm)
from °C to 10°C
from 10 °C to 20 °C
from °C to 30°C
25 – 35 minutes
20 – 30 minutes
15 – 20 minutes
5 – 6 minutes
4 minutes
P80 - P120 - P240
30 minutes
5 vol
D821
1 vol
MS-Hardener
1 vol
Thinner
3 vol
D821
1 vol
DG
1 vol
MS-Hardener
1 vol
Thinner
35 minutes
1,5 - 2 hours (tinted: 2 – 2.5 hours)
Overnight
20 – 25 minutes; tinted: 30
minutes (metal temperature)
10 - 15 min
2,5 % - 3,0 %
from ,0°C to 2,5°C
from ,5°C to 2,0°C
(by weight)
3 vol
1 vol
1 vol
3 vol
1 vol
1,5 vol
1 vol