aluminum, are not to be considered to have changed the surface of the metal.
(2) Cadmium and silver plated fasteners must not be used in or around titanium or its alloys, due to accelerated
embrittlement of titanium caused by these metals.
(3) A metal listed under two or more Group headings is compatible with all of the other metals listed in each of those
groups and with itself. However, metals listed in the same group with a material which is under two different group
headings must be considered incompatible with any of the other metal listed in the second group.
NOTE:
(4) For steels, refer to note at the bottom of Table 3.
Table 4. Recommended Dissimilar Metals Protection
Group From Table 2I
Temperature Range
Interior/Exterior
Group I below 250°F (120
°C) Interior
Group I below 350°F
(177°C) Exterior
Group II below 250°F
(120°C) Interior
Group II 250 to 350°F (120
to 177°C) Interior
Group II below 350°F
(177°C) Exterior
Group III Below 350°F
(177°C)
Group IV Below 350°F
(177°C)
Group IV 350 to 500°F
(177 to 260°C)
Group IV
C. Protective Treatment for Fastener Installation
Copyright © Textron Aviation Inc.
Retain printed data for historical reference only. For future maintenance, use only current data.
Chrome plate is listed under Groups C and D, so it is compatible with a total of 19 other metals.
But the other metals in group C, such as Martensitic stainless steels, are incompatible with all
of the other metal listed in Group D.
Not Exposed to Fuel
Anodize or Protective Treatment and apply
Corrosion Protection Primer
Anodize or Protective Treatment and apply
Corrosion Protection Primer
Aluminum - chemical film and apply
Corrosion Protection Primer Other Group II
- Solvent wipe, manual deoxidize and
apply Corrosion Protection Primer
Aluminum - chemical film and apply
Corrosion Protection Primer Other Group II
- Solvent wipe, manual deoxidize and
apply Corrosion Protection Primer
Aluminum - chemical film and apply
Corrosion Protection Primer Other Group II
- Solvent wipe, manual deoxidize and
apply Corrosion Protection Primer
Lead - sandpaper as needed,
pretreatment prime, apply Corrosion
Protection Primer.
Nickel and diffused nickel, cadmium -
solvent wipe, abrasive clean and apply
Corrosion Protection Primer.
Stainless steel and tungsten - solvent
wipe, abrasive clean and apply Corrosion
Protection Primer
All but graphite. Solvent wipe, abrasive
clean and apply Corrosion Protection
Primer
All but graphite. Solvent wipe, abrasive
clean and seal with RTV 106
Graphite composites. Layer of 181
fiberglass bonded to graphite
FOR TRAINING PURPOSES ONLY
ISSUE 02 , JAN 2018
Model 510 Structural Repair Manual (Rev 2)
51-20-01-0 (Original Issue)
Exposed to Fuel
Anodize or Protective Treatment and apply
Fuel and Corrosion Protection Primer
Anodize or Protective Treatment and apply
Fuel and Corrosion Protection Primer and
topcoat with urethane enamel
Same, but use Fuel and Corrosion
Protection Primer
Same, but use Fuel and Corrosion
Protection Primer
Same, but use Fuel and Corrosion
Protection Primer
Same, but use Fuel and Corrosion
Protection Primer
Same, but use Fuel and Corrosion
Protection Primer
Same, but use Fuel and Corrosion
Protection Primer
Same, but use Fuel and Corrosion
Protection Primer
Same
Same